Takes a killer edge and seems to be more stable then s110v.

Heat treatment
1530f preheat 5min
2150f Austenizing for 10min
Plate quench
Immediate Cryo 4 hours (no snap temper)
3x tempers at 1000f for 2 hours.
I got 64.5rc
Using Larrin's Catra predicting Formula
-−157+15.8×64.5−17.8×30+26.2×23
930 Predicted Total cards cut with 64.5 rc with a 15dps, 30 inclusive angle
I'm closer to 12dps in the video.
That would increase TCC to 1037!
S90v by comparison is
−157+15.8×59−17.8×30+26.2×9+14.6×13
666 TCC with a 59rc and 30 inclusive angle.
682 at 60rc